Description

Main characteristics and applications

WW.NR. 1.2085 is used for core parts and mould bases of corrosion resistance plastic moulds or where equipment needs to be made with excellent workability and excellent corrosion resistance.

Comparable standards
DIN W.Nr AFNOR AISI/SAE JIS
-1.2085 ~Z33CS16 ~442+S -
Chemical composition (typical; in weight %)
C SiMn P (max) S (max) Cr Mo Ni
0.28-0.38 <1.00 <1.40 0.030 0.05-0.10 15.00-17.00 - -

Production technology

EAF – LF – VD – Forging – Heat treatment QT

US specification

In according to standard EN10228-3 Class 4 and standard SEP 1921 Class E/e

Delivery condition

WW.NR. 1.2085 is delivered in quenched and tempered condition, with hardness range 280 – 325 HB (29 – 35 HRC).

Physical properties (reference values)
20°C 100°C 250°C 500°C
Thermal expansion coefficient (10-6/K) 10.5 10.7 12 13.2
Thermal conductivity (W/mk) 22.2 22.7 21 24.5
Young modulus (Kn/mm2) 215 211203 180
Critical points
Ac1 790 °C
Ac3 890 °C
Ms 190 °C
Heat treatment
TREATMENT TEMPERATUREHOLDING TIME (HT) COOLING COMMENTS
Annealing Heat to 850 - 880 °C Min. H.T. for 2 minute /mm Air or furnace In order to obtain hardness lower than 250 HB ( 24 HRC) to improve machinability
Stress relieving Heat to 590 - 650 °C Min. H.T. for 2 minute /mm Air or furnace To be carried out after machining, is recommended to eliminate the residual stresses induced by mechanical working
Hardening Heat to 1000-1050°C Min. H.T. for 1 minute /mm Air or Polymer (depending of size) -
Tempering Heat to 550 – 610°C Min. H.T. for 3 minute /mm Air of furnace To be carried out after hardening. 2nd Tempering must be performed to max 30°C below tempering temperature
size chest(in.) waist(in.) hips(in.)
XS 34-36 27-29 34.5-36.5
S 36-38 29-31 36.5-38.5
M 38-40 31-33 38.5-40.5
L 40-42 33-36 40.5-43.5
XL 42-45 36-40 43.5-47.5
XXL 45-48 40-44 47.5-51.5

Related Products

Featured Products